| Material | Machine | Op | Power | Speed | Passes | DPI | Air | Confirmed |
|---|---|---|---|---|---|---|---|---|
| Black anodised aluminium1.5mm · Diode One pass only. A second pass breaks through to bare metal and goes grey. | LP4 | mark | 100% | 20 mm/s | 1× | 1000 | ||
| Glass (wet paper coated)Diode Wet newspaper mask, air assist OFF or the paper dries mid-job. | LP4 Safeguard | mark | 60% | 42 mm/s | 1× | — | — | |
| Powder-coated tumblerDiode This is paint removal, not metal marking. Lower power than you'd think. | LP4 | mark | 70% | 120 mm/s | 1× | 800 | ||
| Black anodised aluminium1.5mm · Diode Photo work with Stucki dither. Compress tonal range before export. | LP4 | mark | 100% | 15 mm/s | 1× | 1000 | ||
| Coated aluminium business cardDiode Wipe with IPA before and after — fingerprints show as blotches. | LP2 Plus | mark | 100% | 25 mm/s | 1× | 1000 | ||
| Powder-coated tumblerDiode Rotary at 20oz straight wall. Wipe with IPA after. | LP2 Plus | mark | 75% | 100 mm/s | 1× | 800 | ||
| Glass (marking spray)Diode Slightly defocus (0.5mm) to spread the spot and avoid chipping. | LP4 | mark | 55% | 50 mm/s | 1× | — | — | |
| Ceramic tile (glazed)Diode Works on light glaze; dark glaze barely marks. Test the exact tile. | LP4 Safeguard | mark | 100% | 60 mm/s | 1× | 800 |